The short answer

Most dextrin core glue problems trace back to one step in the method: how fast the powder went in, the order of borax and caustic, how much water, how long the glue stood, or how clean the tank was. Read the symptom, find the step, then fix the step rather than adjusting the recipe at random. A batch log (see dextrin glue for paper tubes and cores) makes the cause easy to find.

Symptom finder

Symptom Most likely cause First check
Lumps, fish-eyes Powder added too fast or onto still water [1, p. 269] Addition rate, stirrer vortex
Deep brown glue, little tack Caustic added before borax dissolved [1, p. 281] Batch log: borax and caustic order and times
Rubbery balls, glue will not spread Borax into a thick paste, or too much borax [1, p. 269] Borax pre-dissolved? Weighed?
Sour smell, glue thinner by morning Bacterial souring of standing glue [1, pp. 371–373] Batch size, tank cleaning, preservative
Thicker or cloudy after standing “Set-back” (retrogradation) [1, pp. 216, 281] Time since mixing, dextrin grade
Strings and splatter on the winder Viscosity too high or low, cold glue, or air in the line [2] Viscosity with a calibrated cup
Skin on the glue pot Exposure to air and heat [2] Pot cover, top-ups, line speed
Buildup on the mandrel and cutter Over-application, slow set, or long cleaning intervals [2] Coat weight, cleaning schedule
Cracked, brittle glue film High sugar (dextrose) in the dextrin, or over-dry conditions [1, p. 285] Dextrin COA (reducing sugars), shed humidity
Brown stain on light paper Alkali darkening, iron contamination or some additives [3][1, p. 282] Glue pH, iron contact, additives

In the glue kitchen

Lumps and fish-eyes

Dextrin wets on the outside first. If powder lands in a heap, the outer layer gels and seals the dry powder inside. The starch literature notes that even when powders are sifted onto stirred water, “small lumps are apt to form and give rise to a heterogeneous paste” [1, p. 269].

Fix: start the stirrer first, add the powder gradually into the vortex, and keep stirring until no fish-eyes remain. Do not dump caustic flakes either: add caustic as a dilute solution.

Deep brown glue with poor tack

This is “burnt” glue. Borax must be added first and dissolved before caustic soda. If the order is reversed, the glue “loses most of its adhesive characteristics and turns a very deep brown colour” [1, p. 281]. Alkali darkens dextrin glues in general, especially at high pH [3].

Fix: dissolve the borax completely first, then add the caustic slowly as a solution. A burnt batch rarely recovers, so remake it.

Rubbery balls

Borax raises the viscosity of starch pastes strongly. Added to a starch paste, it can make the mass “like rubber”, so that it “balls up” when spread [1, p. 269].

Fix: pre-dissolve the borax and add it while the batch is still fluid. Weigh it. Too much borax also causes stringing.

Thin, sour or smelly glue

Starch glue is water and carbohydrate, which bacteria can use. Bacterial activity increases once starch is mixed with water. In sizing practice, residual paste left in a vat to cool below about 40 °C between batches “constitutes a good medium” for microbial growth. Bacilli in that residue are “capable of hydrolysing and souring the starch” [1, pp. 371–373]. The glue thins, smells and loses tack.

Fix:

  • Mix what one or two shifts will use.
  • Empty and clean the tank and lines between batches. The starch literature stresses “scrupulous cleanliness” [1, p. 372].
  • If glue must stand longer, use a preservative that is suitable for your market. For US food packaging, check the permitted list (see 21 CFR 175.105 and dextrin adhesives).

Glue that thickens on standing

Some dextrin solutions increase in viscosity with age and show “retrogradation” or reversion, becoming cloudy or pasty. Generally, the further a dextrin is converted, the more stable it is, “although this applies less to mixtures containing caustic soda and borax” [1, p. 216]. The trade calls this “set-back” [1, p. 281].

Fix: use glue within its working life, keep the temperature steady, and check viscosity before each use. If it keeps happening, ask for a more converted dextrin and compare set-back on a sample.

On the winder

Stringing and splatter

A core-winding supplier links stringing and splatter to viscosity that is too high or too low, cold adhesive, or air in the supply line [2]. Excess borax also makes glue stringy.

Fix: measure viscosity with a calibrated cup “rather than by eye” [2], warm the glue to the method temperature, and bleed air from the lines.

Skinning in the pot

Glue exposed to air and heat dries on the surface and on the rollers. The same supplier recommends checking reservoirs and applicators every shift for “skinning or dried film” [2]. Skinned glue is a common cause of ply separation [2].

Fix: cover the pot, top up little and often, and clean the applicators every shift. In dry inland summers, expect more skinning (see paper core moisture).

Buildup on the mandrel and cutter

This usually comes from over-application, slow-setting glue or a cleaning interval that has stretched out. It also shortens blade life [2].

Fix: check the coat weight and the cleaning schedule. If the glue is slow to tack, look at its solids and borax level.

Cracked, brittle glue film

Dextrose is more hygroscopic than maltose, and a dextrin with too much of it gives a glue film that dries fast on the surface. The internal strain then makes the film crack [1, p. 285].

Fix: check reducing sugars on the dextrin COA, and compare lots. Very dry shed air makes the problem worse.

Stains on light paper

On brown kraft cores, glue colour does not matter. On white or light paper, a brown line can come from:

  • the colour of a yellow dextrin;
  • alkali in the glue darkening over time, which is worst above about pH 10 [3];
  • iron contamination, which causes “intense discoloration” with some additives [1, p. 282].

See white vs yellow dextrin for which dextrin to use where colour shows.

Make it a symptom card

Print the symptom finder table and pin it at the mixer and the winder. When a problem appears:

  1. Write the symptom in the batch log.
  2. Check the one step the card points to.
  3. Change only that step in the next batch.
  4. Record the result.

The U.S. Borax technical bulletin warns that “a formula working well on one machine will fail on another” [4]. Change one thing at a time.

FAQ

Why does my dextrin glue turn brown? Usually because caustic soda went in before the borax had dissolved, or too fast [1, p. 281]. High pH in general darkens dextrin glues [3].

Why does my core glue smell sour? Bacteria are souring glue that has stood too long or was mixed in a dirty tank [1, pp. 371–373]. Mix smaller batches and clean the tank.

Why does my glue get thicker overnight? That is set-back (retrogradation) of the starch in solution [1, p. 216]. Use the glue within its working life, or test a more converted dextrin.

Why do my cores separate between plies? Often a coat-weight or set-time problem, including skinned glue [2]. See our guide on returned cores: crush failure or ply separation.

Same problem every week? Send us your symptom, your batch log and a photo of the glue. Shalbond makes yellow dextrin and paper tube gum powder in India, and we will suggest the step to check, with a 1 kg lab sample, TDS and COA if a powder change is worth testing. Send your details or message us on WhatsApp at +91 89897 00688.

Need a Specific DE Value
or Compliance Certificate?

Our food science team will match your exact specification and send a 1kg lab sample with full COA within 48 hours. No minimum order for initial qualification.

💬