Dextrin Glue for Paper Tubes and Cores: Order of Addition, Borax and Caustic
The short answer
Most dextrin core glues are made on site from dextrin, water, borax and caustic soda. Three habits decide whether the glue is the same every batch:
- Dissolve the borax completely before adding any caustic soda, then add the caustic slowly. If caustic goes in first, the glue “burns”: it turns deep brown and loses most of its tack [1, p. 281].
- Weigh everything, every time, including the water. Glue made by the scoop drifts.
- Measure viscosity at the end of every batch with the same cup and at the same temperature, and write it down.
If you are moving from synthetic glue, or nobody has given your plant a written method, the sections below explain what each ingredient does and how to build a method you can repeat. We do not publish ratios here, because the right amounts depend on your dextrin, board, winder speed and climate. Ask for a written method matched to the powder you use.
What each ingredient does
| Ingredient | Job in the glue | What goes wrong if it is off |
|---|---|---|
| Yellow dextrin | The adhesive. A well-converted dextrin dissolves at high solids and gives a sticky gum that does not soak into absorbent tube board [1, p. 280]. | Low or variable cold-water solubles give thick, lumpy or weak glue. |
| Water | Carries the dextrin. Less water means less penetration into the board and less to dry out of the core [1, p. 280]. | Too much: slow drying, wet cores, soft crush strength. Too little: glue too thick to run. |
| Borax | Links starch chains into a larger, more branched polymer, raising viscosity and giving quicker tack for high-speed machines [2]. It also buffers the action of caustic soda [1, p. 281]. | Too much, or added to a thick paste: rubbery lumps and stringing. Borax added to a starch paste can make it “like rubber” so that it “balls up” when spread [1, p. 269]. |
| Caustic soda | Works with borax to build the branched polymer that gives wet tack [3]. Alkali in the mix also improves stability and wetting of hard-to-wet surfaces [1, p. 286]. | Added before the borax, or too fast: burnt, brown glue with poor tack [1, p. 281]. Too much: darkening and stains. |
| Preservative (if used) | Stops bacteria souring glue that is kept for more than a shift. | Without it, warm glue can sour and thin overnight (see core glue troubleshooting). |
In tube winding, the borax-and-alkali system is not optional decoration. A European Commission study of borate uses records that borax with a small amount of sodium hydroxide makes starch into a more branched, higher-molecular-weight polymer that improves wet tack. It also improves film forming and holds enough water for the bond to form [3, p. A5-1]. The same study reports industry’s view that there is “no direct alternative technology commercially available” for borax in tube winding without rebuilding factories [3, p. A5-5].
Why the order of addition matters
The starch technology literature is direct: borax “should always be added first and allowed to dissolve before the addition of caustic soda. If these compounds are added in the reverse order the glue becomes ‘burnt’, i.e. loses most of its adhesive characteristics and turns a very deep brown colour” [1, p. 281].
The reason is the borax buffer. Dissolved borax moderates the effect of the caustic [1, p. 281]. Without it, strong alkali hits the dissolved dextrin directly, and alkali is known to darken dextrin glues severely, especially at high pH [4].
Two other order problems cause most of the remaining bad batches:
- Powder dumped into water forms lumps. Even when powder is sifted onto stirred water, “small lumps are apt to form and give rise to a heterogeneous paste” [1, p. 269]. Add the dextrin gradually into a strong vortex, and do not add it all at once.
- Undissolved borax or neat caustic gives local over-reaction. Pre-dissolve borax in warm water and add caustic as a dilute solution, never as flakes, so no part of the paste sees a high local concentration.
A mixing sequence that gives the same glue every batch
This sequence is a framework. Your written method should add the weights, temperatures, mixing times and target viscosity for your dextrin.
- Charge and weigh the water. If you heat with live steam, mark the tank and allow for condensed steam, which adds water to the batch [1, p. 280].
- Start the stirrer, then add the dextrin gradually into the vortex. Keep stirring until no lumps or “fish-eyes” remain.
- Bring the batch to the method temperature if your method uses heat, and hold it for the stated time.
- Add the borax as a solution and stir until it has fully dissolved and mixed in.
- Add the caustic slowly, as a dilute solution, with the stirrer running. Watch the colour: a sudden darkening means it went in too fast.
- Add any preservative or other additives last, as your method states.
- Cool if required, then measure viscosity with the same cup or viscometer, at the same temperature, every batch.
- Strain into the glue pot. Record the batch in the log.
The U.S. Borax technical bulletin makes an important point: “A formula working well on one machine will fail on another” [2]. Treat your first method as a starting point, and adjust it on your own winder by changing one thing at a time.
Keep a batch log
A batch log turns “the glue was bad today” into a cause you can find. Pin it at the mixer.
| Field | Why it matters |
|---|---|
| Date, shift, operator | Links problems to people and times without guesswork |
| Dextrin lot number | Separates powder variation from mixing variation |
| Water weight and start temperature | The biggest single cause of viscosity drift |
| Dextrin weight | Confirms nobody scooped |
| Time borax added, and “fully dissolved?” (yes/no) | Catches order-of-addition errors |
| Time caustic added, and how (solution, slowly) | Catches burnt batches |
| End viscosity (cup, temperature) | The number that tells you the glue is the same |
| Shed temperature and humidity | Explains seasonal drift in drying and tack (see paper core moisture) |
| Notes: colour, smell, lumps | Early warning of souring or burning |
When a delivery of dextrin arrives, compare it with a retained standard sample for viscosity in solution, colour and stability before you use it. The literature recommended this decades ago [1, p. 281], and it still prevents most “the new powder is bad” disputes.
Dextrin plus a glue kitchen, or a one-bag gum powder?
There are two ways to run starch core glue, and both work.
| Dextrin + borax + caustic on site | One-bag tube or core gum powder | |
|---|---|---|
| What you buy | Dextrin, plus borax and caustic from local suppliers | One powder; add water |
| Control | Full: you can tune tack and viscosity | Less: the blend is fixed |
| Consistency risk | Order-of-addition and weighing errors | Lower mixing risk; still depends on water and stirring |
| Sourcing | Borax is not always easy to buy locally | No borax or caustic to source separately |
| Handling | You handle caustic and borax in the plant | The powder itself contains alkali and borate, so it needs an SDS and careful handling |
| Best for | Established plants with a written method and someone who owns the glue kitchen | New plants, small lines and plants without a fixed recipe |
Whichever route you choose, judge it by a side-by-side trial on your winder, with the same board and the same drying conditions, comparing crush strength at the same core moisture.
Safety and regulatory notes
- Caustic soda is corrosive. Wear eye protection and gloves, add caustic to water and never water to caustic, and follow the supplier’s safety data sheet.
- Borax has a harmonised EU classification as toxic for reproduction (Repr. 1B, H360FD) at specific concentration limits [5]. If your tubes or cores go to EU customers, check whether that affects your documents, and ask your glue supplier for an SDS that reflects it.
- Get an SDS for every powder that contains borax or caustic before it arrives at your plant.
When the glue still goes wrong
| Symptom | Most likely cause | First check |
|---|---|---|
| Lumps or fish-eyes | Powder added too fast | Addition rate and stirrer vortex |
| Deep brown glue with poor tack | Caustic before borax was dissolved, or added too fast | Log: borax and caustic times |
| Rubbery balls, glue will not spread | Borax into a thick paste, or too much borax | Borax dissolved first? Weighed? |
| Long strings, splatter | Viscosity too high, or excess borax | End viscosity vs target |
| Sour smell, thinner by morning | Bacterial souring | Batch size, preservative, tank cleaning |
Each of these is covered in detail in our paper core glue troubleshooting guide.
FAQ
Can I make dextrin core glue without borax? Some glues are made without it, but borax is what gives the quick tack and viscosity that most winders rely on [2][3]. Removing it usually means changing the dextrin, the solids and the machine settings, so trial it carefully.
Why is my glue brown even though I use the same dextrin? Check the order and speed of caustic addition first. Alkali added before the borax has dissolved, or too fast, burns the glue [1, p. 281]. Yellow dextrin glue is also naturally amber, which does not matter on kraft cores.
How do I know a new batch is right before it reaches the winder? Measure end viscosity with the same cup at the same temperature, and compare it with your target. Then check that the colour and smell are normal. These three checks catch most bad batches.
Should I mix one big batch for the week? No. Starch glue can sour and change viscosity on standing. Mix what one or two shifts use, unless your method includes a preservative and you have tested its stability.
Want a written method for your powder? Shalbond makes yellow dextrin for tube and core glue and a one-bag paper tube gum powder in India. Tell us your board weight, number of plies and winder, and we will send a 1 kg lab sample with TDS and COA, plus a mixing method to trial. Send your details or message us on WhatsApp at +91 89897 00688.