The short answer

When warp breaks rise, check the loom-shed humidity before you change the size recipe. In a mill study on cotton warps, breaks were lowest at about 84–85% relative humidity. Below that, the size film cracked. Above it, the size softened and was scrubbed off the yarn [1].

Once humidity is right, look at the size. It must penetrate the yarn enough to bind the fibres, and coat it enough to lay the hairs and resist abrasion [2, pp. 324–325]. Thin-boiling (acid-modified) starch is used because its lower viscosity helps the size penetrate at useful solids [2, p. 325].

Start with shed humidity

A 2017 study on 10 air-jet looms weaving 60s cotton found that warp breakage is “highly sensitive to the relative humidity” [1]:

Shed RH What happened
About 80–83% Size film cracking, more warp breaks, lower efficiency
About 84–85% Lowest breaks and highest loom efficiency in that mill
Above about 85% “Size coating soft and scrubbed off from the yarn”; bare yarn breaks

The study cites 80–85% RH as a general textile-mill standard for cotton fabrics [1]. It covers one fabric, one plant and about a month, so your best point may differ. The direction is clear, though: too dry and too wet both raise breaks. A trade overview also lists RH, alongside yarn quality, sizing, loom settings and abrasion, among the main factors in end breakage [3].

What to do: log shed RH and temperature beside warp stops per loom per shift for two to four weeks. If breaks track the humidity, fix the humidification before touching the size.

What the size must do: penetrate and coat

The starch technology literature describes “two schools of thought”: one keeps the size on the surface, the other wants it to penetrate the yarn [2, p. 324]:

  • Size held only on the surface “is apt to be mechanically removed, or ‘dust off,’ in the weaving”.
  • Penetration gives better extensibility, which reduces breakages, because the size film is less extensible than the fibre.
  • The practical answer is a size “which combines a certain degree of penetration with adequate surface protection” [2, pp. 324–325].

Viscosity controls that balance. A thick size sits on the surface; a thinner one penetrates. Paste viscosity also depends on the starch source: potato starch gives a more viscous paste than maize, weight for weight [2, p. 325].

Where thin-boiling starch fits

“A converted or modified starch is used to obtain penetration, because the viscosity of solutions of these preparations is much less than that given by untreated starch” [2, p. 325]. Thin-boiling starches are acid-modified, so they cook to a lower viscosity at the same solids.

The degree of thinning is traditionally expressed as fluidity: the volume of a standard starch solution that flows from a pipette in a set time. That is where names like “90 fluidity” or “60 fluidity” thin-boiling starch come from [2, p. 325]. Higher fluidity means thinner.

Two cautions from the same text [2, p. 325]:

  • Over-modified starch gives weaker films. Film strength from cooked native starch can exceed that from “modified thin-boiling starches that have received excessive treatment”, at the same add-on. More fluidity is not always better.
  • Consistency matters. “When a supplier of a satisfactory thin-boiling starch has been found”, it is safer to keep buying from them than to try to match the quality by modifying starch at the mill.

Size also has to come out again. Fabrics are desized before dyeing, so the size must be removable (residual size can act as a resist and cause dyeing faults) [2, p. 324].

A warp-break checklist

Check What to look for
Shed RH and temperature Logged hourly; compare with breaks per shift [1]
Yarn Count, strength, unevenness, hairiness from the spinning mill [3]
Size viscosity Measured at the sow-box temperature, every set
Size add-on (pick-up) Within target; it varies with viscosity and squeeze pressure [3]
Penetration vs coating Cross-section or abrasion test on sized yarn
Size film Cracking or dusting at the loom
Loom settings Shed depth, timing and tension [3]
Starch lot A new lot or supplier just before the change

FAQ

What humidity should a loom shed run at for cotton? A general standard of 80–85% RH is often cited. One mill study found the fewest breaks at 84–85% [1]. Find your own point by logging RH against breaks.

Why does sized yarn break more in dry air? The size film becomes brittle and cracks, and the yarn loses moisture and elasticity [1].

What is thin-boiling starch used for in textiles? Warp sizing, where its lower viscosity helps the size penetrate the yarn at useful solids [2, p. 325]. It is also used in some finishes where a thin, clear film is wanted [2, p. 326].

What does “fluidity” mean for thin-boiling starch? A measure of how far the starch has been thinned, based on how much of a standard solution flows in a set time. Higher fluidity means lower viscosity [2, p. 325].

Humidity under control and still breaking? Shalbond makes thin-boiling starch for warp sizing in India. Tell us your yarn count, size recipe and target viscosity, and we will send a 1 kg lab sample with TDS and COA. Request a sample or message us on WhatsApp at +91 89897 00688.

Need a Specific DE Value
or Compliance Certificate?

Our food science team will match your exact specification and send a 1kg lab sample with full COA within 48 hours. No minimum order for initial qualification.

💬