Stein-Hall Corrugating Adhesive Explained: Carrier, Raw Starch and Gel Point
The short answer
A Stein-Hall (carrier) corrugating adhesive is “a suspension of ungelatinized starch particles in a thin paste of gelatinized starch, called the carrier phase” [1]. The cooked carrier keeps the raw starch suspended and gives the glue body. On the corrugator, heat gelatinises the raw starch in place, and that forms the bond. Caustic soda lowers the starch’s gel point; borax builds tack and buffers the caustic [1][2].
The two numbers to control every batch are viscosity and gel temperature. The right values depend on your corrugator speed, preheat and paper.
Two starches in one glue
| Part | What it is | Job |
|---|---|---|
| Carrier | A fraction of the starch, gelatinised with caustic soda [2] | Suspends the raw starch; gives viscosity and initial tack |
| Raw (secondary) starch | Uncooked starch granules in suspension [1] | Gelatinises on the machine under heat, forming the bond |
The U.S. Borax bulletin describes the carrier as “gelatinizing a fraction of the total starch by caustic soda” to keep the rest of the granules in suspension. On the machine, the starch applied to the flute tips “swells under machine heat”, bonding the medium to the liner in place [2].
What caustic does
- Gelatinises the carrier fraction [2].
- Lowers the gel point of the raw starch: “The strong base also lowers the gel point of the starch” [1]. That lets the bond form at the temperature and speed of the machine.
Too much caustic, or caustic added too fast, can over-gelatinise the carrier or darken the glue. Alkali darkening of starch and dextrin glues is well documented [3].
What borax does
- Forms a starch–borax complex that helps gel the starch and increases tack [1].
- Buffers the caustic, stabilising the adhesive against hydrolysis [1].
- Gives “increased viscosity, quicker tack and better fluid properties” for high-speed machines [2].
Gel point: the number that matters on the machine
Every starch has a gelatinisation temperature at which its granules swell irreversibly. For starches generally, this is about 55–80 °C, depending on the starch and its concentration [4, p. 12]. The higher the concentration, the lower the apparent pasting temperature [4, p. 15]. In a corrugating adhesive, the gel point of the raw starch is lowered by caustic [1]. The examples in one corrugating patent show gel points of roughly 141–146 °F (about 61–63 °C) [1].
Why it matters:
- Gel point too high: the raw starch does not gelatinise fully at machine speed, which gives weak bonds or “zippers”.
- Gel point too low: the glue starts to gel in the pan or on the rolls, thickening and building up.
Machine speed, preheat and paper temperature decide the right gel point for your line. Measure it every batch.
How much glue goes on the board
FEFCO gives typical glue consumption per glue layer by flute [5]:
| Flute | Glue per glue layer (g/m²) |
|---|---|
| A | 4.5–5.0 |
| C | 5.0–5.5 |
| B | 5.5–6.0 |
| E | 6.0–6.5 |
| F, G, N | 9.0–11.0 |
A single-wall board has two glue layers. Excess glue wastes starch and adds water to dry. Too little gives weak bonds.
What to measure every batch
| Check | Why |
|---|---|
| Viscosity (Stein-Hall or other cup, same temperature) | Pickup and penetration on the glue rolls |
| Gel temperature | Bond formation at machine speed |
| Solids | Water load into the board |
| Temperature in the storage tank | Stability before use |
| Viscosity after a stop | Pot-life and resin effects. Adding resin can cause a sharp viscosity rise (“resin shock”), which in borated carrier adhesives “can be permanent” [1]. |
For how cups compare with other viscometers, see measuring glue viscosity.
FAQ
What is a Stein-Hall adhesive? A carrier-type corrugating adhesive: a cooked starch carrier that suspends uncooked starch, which gelatinises on the corrugator [1][2].
What does caustic soda do in corrugating glue? It gelatinises the carrier and lowers the gel point of the raw starch [1][2].
What is gel point? The temperature at which the raw starch swells and gels. It must match your machine’s heat and speed.